A study of natural pigment-based colour masterbatches has found that four commercial bio-based colorants can be processed with polylactic acid (PLA) and polybutylene succinate (PBS) on conventional twin-screw compounding and injection molding equipment, with only modest effects on melt flow and mechanical performance. Colour stability under light remains the principal limitation.
The work, set out in a study titled "Sustainability in the Development of Natural Pigment-Based Colour Masterbatches and Their Application in Biopolymers," used blue spirulina, yellow curcumin, red beetroot and green chlorophyllin. Each pigment was combined with PLA or PBS to make masterbatches by twin-screw extrusion, then diluted into the matching polymer at 2, 4 and 6 wt% and injection molded into test specimens. Titanium dioxide, calcium carbonate and stearic acid were included in the formulation to support UV protection, dispersion and processing.
Thermal limits define the processing window
Because the organic structures of natural pigments can degrade at temperatures below those at which the polymers soften, thermogravimetric analysis was used to establish onset temperatures: approximately 229 °C for spirulina, 244 °C for curcumin, 258 °C for chlorophyllin and 267 °C for beetroot. PLA and PBS degrade at considerably higher temperatures.
The researchers therefore selected extrusion profiles that melted each polymer while limiting the pigments' heat exposure, reaching 145 °C for PBS and 190 °C for PLA, with the twin-screw extruder running at 65 rpm and a feed rate of 2 kg/h.
Most pigment–polymer pairs tolerated this window. Spirulina was the exception: during PLA processing it lost its characteristic blue, so a blue PLA masterbatch could not be produced. The lower processing temperature used for PBS left the same pigment stable enough for successful compounding, indicating that compatibility depends heavily on the thermal demands of the matrix rather than on the colorant alone.
Melt flow and mechanics stay near baseline
Melt flow rate declined slightly after pigment incorporation, pointing to a small increase in melt viscosity. Neat PLA measured about 50 g/10 min, and the corresponding natural-pigment masterbatches remained close to that figure; PBS responded in similar fashion. For compounders this is significant, since a colour system that demanded major alterations to screw design, pressure settings or molding conditions would have little practical value. Here most formulations ran through standard equipment without major processing problems.
Tensile and impact testing across the 2 to 6 wt% range showed no significant overall losses. PLA started from a Young's modulus of about 1710 MPa and tensile strength of 65.6 MPa, PBS from roughly 392 MPa and 34.5 MPa. The coloured formulations stayed close to those baselines, and impact strength remained in a comparable band, although individual pigments produced some variation.
Photostability is the largest gap
Successful extrusion did not guarantee lasting colour. After 50 hours of xenon-lamp exposure, most formulations exceeded a colour difference of ΔE* = 2, the level at which a change becomes visually perceptible. The clearest exception was PLA containing 2 wt% green chlorophyllin masterbatch, which showed the highest photostability.
The study accordingly identifies UV stability as the main barrier to broader use. Packaging, consumer products, agricultural parts and outdoor applications may require additional stabilisation, protective coatings or pigment modification before natural colours can compete with conventional systems over long service periods.
Lower footprint, but development continues
On the environmental side, the study's assumptions put one kilogram of curcumin pigment at about 0.04 kg CO2-eq, compared with 18.65 kg CO2-eq for the inorganic green reference pigment, and the natural-pigment masterbatches also consumed less electricity during extrusion and pelletizing.
The researchers conclude that lightfastness and thermal stability need further development, while noting that several natural colorants can be compounded into PLA and PBS with conventional equipment and with only limited changes in melt viscosity and mechanical behaviour. Future work, they suggest, should concentrate on colour stability both during processing and in subsequent service exposure.